A formulator moves a spray polyurea B-side from a 2000-weight diamine to polyetheramine D-4000 for more elongation. The batch sheet takes the grade’s amine hydrogen equivalent weight (AHEW), 1000 g/eq, and runs it against the prepolymer. The same grade also has an equivalent weight with isocyanates: 2000 g/eq.
The B-side now delivers half the amine equivalents the index assumed. The panel cures, the isocyanate excess goes looking for moisture, and the trial gets written off as a bad lot. Nothing was wrong with the lot.
Which polyetheramines go into polyurea and RIM, and which number sets the ratio?
Polyetheramines for polyurea and reaction injection molding (RIM) are long-chain polyoxypropylene amines: diamines at Mn ≈ 2000 and Mn ≈ 4000, a triamine at Mn ≈ 5000, and a secondary diamine for slower cure. Against isocyanate, the ratio runs on the isocyanate equivalent weight, which for RS-D4000 is 2000 g/eq, double its AHEW.
The polyoxypropylene diamine at Mn ≈ 2000, polyetheramine D-2000 on public pages, is the reference grade here. It is a key ingredient in polyurea and RIM formulations. The other three grades share its polyether backbone and differ in chain length, functionality or amine substitution, and the urea-relevant lines differ from grade to grade. The polyetheramine family overview covers the short-chain epoxy grades. This piece stays on the isocyanate side.
Why does an epoxy number break a urea calculation?
AHEW counts hydrogens. A primary amine group carries two, and in an epoxy cure both open an oxirane ring. That is why the polyoxypropylene diamine at Mn ≈ 2000 has an AHEW of 505 g/eq: the number is built for an epoxy resin, where every N-H counts.
Isocyanate behaves differently. The first N-H on a primary amine reacts with an NCO group to form a urea. The remaining hydrogen on that urea nitrogen is far less reactive under normal spray or RIM processing, so one amine group consumes one isocyanate group. Equivalent weight against isocyanate is therefore set by amine groups per molecule, not by hydrogens.
RS-D4000 has both: AHEW 1000 g/eq, equivalent weight with isocyanates 2000 g/eq. Both figures are typical values. Every RS-D4000 lot is held to its amine value, 0.44 to 0.52 mmol/g, and the lot COA reports where each lot sits in that range. The typical figure tells you which basis to use. The lot amine value is what the dose rests on.
Here is the position, and where it could be wrong. The isocyanate equivalent weight is the only defensible basis for a polyurea index. It weakens at high index or elevated post-cure temperature, where urea N-H can go on to form biuret and consume extra isocyanate. If your process runs hot or well over index, the effective equivalent weight sits somewhere between the two numbers, and only a trial panel tells you where.
Keep the AHEW where it belongs. In an epoxy, RS-D4000 is charged at 16.7 times the weight of the short-chain RS-D230 against the same resin (1000 ÷ 60), a ratio built entirely on AHEW. Carry that number into a polyurea worksheet and the index is wrong before the first shot.
Action: For RS-D2000, which has an AHEW but no specified isocyanate equivalent weight, base the dose on the lot COA amine value against its 0.98 to 1.10 meq/g specification, on an amine-group basis. Record on the batch sheet which titration method and unit the COA states.
Four grades side by side, each in its own units
The table keeps every value in its grade’s own unit. Amine value is given in meq/g for two grades and mmol/g for the other two; for an amine titration those are the same number, so the row reads straight across. Color is given as APHA for the diamines and Pt-Co for the other two, two names for the same platinum-cobalt scale.
| Property | RS-D2000 | RS-D4000 | RS-T5000 | RS-SD2001 |
|---|---|---|---|---|
| CAS | 9046-10-0 | 9046-10-0 | 64852-22-8 | 81455-53-0 |
| Nominal molecular weight | 2000 g/mol | 4000 g/mol | 5000 g/mol | Approx. 2,000 g/mol |
| Functionality | difunctional primary amine | difunctional primary amine | trifunctional primary amine | difunctional secondary amine |
| AHEW (typical) | 505 g/eq | 1000 g/eq | – | – |
| Equivalent weight with isocyanates (typical) | – | 2000 g/eq | – | – |
| Amine value (specification) | 0.98 to 1.10 meq/g | 0.44 to 0.52 mmol/g | 0.50 to 0.57 meq/g | 0.875 to 1.03 mmol/g |
| Acetylatables (specification) | – | – | 0.58 to 0.63 meq/g | – |
| Primary amine | 97 min wt% | 95.0 min % | 97.0 min wt% | 5 max % |
| Moisture | 0.25 max wt% | 0.25 max % | 0.25 max wt% | 0.20 max % |
| Color | 25 max APHA | 75 max APHA | 25 max Pt-Co | 100 max Pt-Co |
– not specified; ask the desk.
One thing in that table catches buyers: both diamines share CAS 9046-10-0. EPA’s Substance Registry Services record for 9046-10-0 (EPA Substance Registry Services, retrieved October 2026) names it “Polypropylene glycol bis(aminopropyl) ether” and lists it on the TSCA Inventory kept under TSCA section 8(b), 15 U.S.C. 2607(b).
One registry identity covers both chain lengths, so the CAS on a purchase order cannot tell a 2000 chain from a 4000 chain.
Action: Write the RS code and nominal molecular weight on every purchase order for the diamines, and require the lot COA to repeat both.
The triamine carries two assay lines, and the gap between them matters
RS-T5000, polyetheramine T-5000 on public pages, is the crosslinker in many spray polyurea elastomers. Its first application is as a raw material for spray polyurea elastomers and modified polyetheramines. Its amine value is specified at 0.50 to 0.57 meq/g and its acetylatables at 0.58 to 0.63 meq/g.
The ranges do not overlap. Acetylation picks up hydroxyl groups as well as amine groups, so the gap between the two lines reads, as an interpretation rather than a specified value, as residual hydroxyl: chain ends from the parent polyether triol that did not convert to amine. Those hydroxyls still react with isocyanate. They do it slowly, forming urethane rather than urea.
That gap is the most useful number a polyurea formulator gets for this grade. Balance the index on amine value alone and the hydroxyl ends consume isocyanate you did not budget for, so the cured film runs under index. Balance on acetylatables and every isocyanate-reactive group is counted, though the hydroxyl fraction cures on a slower clock than the amine around it.
The registry identity is distinct from the diamines. EPA’s SRS record for 64852-22-8 carries a propanetriyl-tris index name (EPA Substance Registry Services, retrieved October 2026).
That record lists the substance on the TSCA Inventory, the list EPA must compile, keep current and publish under TSCA section 8(b), 15 U.S.C. 2607(b) (EPA Substance Registry Services, retrieved October 2026).
Action: Hold RS-T5000 to both lines on every lot COA, and calculate isocyanate demand from acetylatables. Track the gap lot to lot. A lot with acetylatables at the top of 0.58 to 0.63 meq/g and amine value at the bottom of 0.50 to 0.57 meq/g carries the most slow-curing hydroxyl the specification allows; flag it before it reaches a fast-gel spray line.
When the triamine shares the B-side with a diamine, the blend equivalent weight is a harmonic mean: the reciprocal of the sum of each component’s mass fraction divided by its equivalent weight. A linear average of the two equivalent weights overstates the amine charge, and the error grows as the two numbers diverge.
When is the secondary diamine worth its slower gel?
RS-SD2001 is N,N’-diisopropyl polyoxypropylene diamine, CAS 81455-53-0. EPA’s SRS record for 81455-53-0 also lists it on the TSCA Inventory kept under TSCA section 8(b), 15 U.S.C. 2607(b) (EPA Substance Registry Services, retrieved October 2026).
It is a difunctional secondary polyetheramine derived from the 2000 molecular weight polyoxypropylene diamine. Its relatively low reactivity suits applications that need a slower cure, and its uses include polyurea and polyurethane systems and RIM.
The isopropyl group on each nitrogen does the work. It crowds the amine hydrogen, and the urea reaction slows.
Each secondary amine group still consumes one isocyanate group, so the equivalent count stays close to that of the primary parent at the same chain length. The rate is what moves, and rate governs flow, substrate wetting and how far a RIM shot travels before it gels. The general split between primary and secondary amines is laid out in the overview of amine types, properties and uses.
The trade-off is real. A primary-amine B-side gels fast enough to build film on vertical steel without sag. Swapping part of it for the secondary diamine buys working time and a cooler exotherm, which helps thick sections and complex molds, but it gives back some of the speed that made polyurea worth its cost. Neither choice is free.
Watch primary amine, 5 max %. Residual primary amine is the fast fraction. A lot near that ceiling gels sooner than a lot near zero, and on a tight RIM cycle the shift shows up as short shots or knit lines.
Action: Make primary amine content a lot acceptance line for RS-SD2001, and run a gel-time check on each new lot against your retained qualification sample before it goes to production.
Moisture and color are acceptance lines
Water reacts with isocyanate, forms an unstable carbamic acid and releases carbon dioxide. In spray polyurea that gas becomes pinholes and blisters; in RIM it becomes voids. Moisture is capped at 0.25 max wt% for RS-D2000 and RS-T5000, 0.25 max % for RS-D4000 and 0.20 max % for RS-SD2001.
Packaging follows the same logic. RS-D2000 and RS-D4000 come in 200 kg drums (nitrogen blanketed) or 1,000 kg IBC totes, and RS-D4000 also in ISO tanks. RS-SD2001 comes in 200 kg net drums (nitrogen blanketed) and is stored protected from moisture and contamination. A drum opened for a partial draw and closed under air is no longer blanketed.
Color matters when the elastomer is pigmented light or left clear. The 25 max APHA ceiling on RS-D2000 is tighter than the 75 max APHA ceiling on RS-D4000. Switching grades for elongation can also move the cured film’s starting color.
Action: Test moisture on receipt against each grade’s ceiling for any lot going to spray, rather than relying on the COA alone. Re-blanket partially used drums with dry nitrogen, and retest any drum held open across shifts before it is pumped.
What to write on the RFQ
The isocyanate side gets its own specification. The amine side deserves one written for isocyanate too. In RIM the polyetheramine often shares the B-side with polyether and polyester polyols, and the same equivalent-weight discipline applies to both streams.
- Name the RS code and nominal molecular weight, not CAS alone. The two diamines share 9046-10-0.
- Treat a typical isocyanate equivalent weight as the basis, not the limit. For RS-D4000 the 2000 g/eq figure is typical; hold every lot to the 0.44 to 0.52 mmol/g amine value specification on the COA.
- For RS-T5000, require acetylatables and amine value on every lot COA, and base the index on acetylatables.
- For RS-SD2001, make primary amine content (5 max %) an acceptance line, paired with a gel-time check.
- Set moisture acceptance at each grade’s ceiling, with the unit stated on the COA.
- Require the amine value unit and what was titrated, total or primary amine, on every COA. Read meq/g and mmol/g as the same number, and convert mg KOH/g by dividing by the molar mass of potassium hydroxide.
If the chemistry itself is still open, the comparison of polyurea, polyaspartic and polyurethane raw materials sets out where each one earns its place.
The decision comes down to one column on your batch sheet. If the equivalent weight entered against your isocyanate is a diamine’s AHEW, the index has been wrong since the formula was written, and the next lot will not fix it.
Methodology: each grade value is what the technical data sheet for that RS code states, in its units, typical where marked typical; the lot COA governs. Registry identities and TSCA Inventory listings are from EPA Substance Registry Services records (retrieved October 2026) and TSCA section 8(b), 15 U.S.C. 2607(b); readings of the chemistry (biuret formation, the source of the acetylatables gap) are labeled as readings.
Frequently asked questions
Is polyetheramine D-2000 a low viscosity polyether diamine?
Do polyetherdiamine grades share a CAS number?
Can amine value results on different lot certificates be compared directly?
Does the slower secondary diamine change how much isocyanate the formula needs?
Sources & methodology
Figures are RawSource sourcing data unless attributed to a named source. Regulatory citations are current as of publication. Chemical identities verified by CAS number against the RawSource catalog.
Search 1,300+ industrial chemicals by name or CAS, or send us your spec — we quote by the drum, tote, or container.
Browse the Chemical Index → Request a Quote